    Default Thousands of pimple sized blisters/bubbles on first coat of polyurethane varnish

    Hi all, I’ve just applied the first coat of FeastWatson Weatherproof brand polyurethane timber varnish to a new timber deck railing. For prep I stirred the varnish (gently - not mixing) and brushed the varnish on to a timber surface sanded with 120 grit.

    It was all going swimmingly until I looked back to the end I’d started at and noticed a sea of small bubbles/blisters.

    Have I done something wrong? I intend to put on two more coats and will sand in between, and I’m hoping the bubbles diminish with each coat. Or is my technique fundamentally flawed?

    Regards, Steve.

  2. # ADS
    Google Adsense Advertisement
    Join Date
    Always
    Location
    Advertising world
    Posts
    Many





     
  3. #2
    Join Date
    Feb 2009
    Location
    moonbi nsw Aus
    Age
    69
    Posts
    2,065

    Default

    It sounds like the hand rail is outside and in the sun.....correct?. If it is the little bubbles is a reaction by the warm rail and you brushing on probably cold varnish. It is quite normal. when dry sand the surface to remove the bubbles and reapply the varnish. By the time you have done 3 coats all will be well. The air in the tiny grains of the timber is warm and your varnish being cols draws out the air to form bubbles.

    Bear in mind to keep your hand rail in good condition you should be recoating every couple of years to keep it looking good
    Just do it!

    Kind regards Rod

  4. #3
    Join Date
    Aug 2008
    Location
    Birkdale
    Age
    51
    Posts
    279

    Default

    I think chambezio is on the money. It can also occur if you coat the timber as it is warming up. As it warms up the gasses in the timber expand and bubbles can form in the finish.

  5. #4
    Join Date
    Oct 2004
    Location
    Hobart
    Posts
    51

    Thumbs up

    Quote Originally Posted by chambezio View Post
    It sounds like the hand rail is outside and in the sun.....correct?. If it is the little bubbles is a reaction by the warm rail and you brushing on probably cold varnish
    Spot on chambezio. The varnish was indeed stored in my underhouse workshop which is always cool, and the rails are outside and it’s a sunny day.

    Thank you for the clear and concise explanation (and the added reassurance).

    Thanks again, Steve.

  6. #5
    Join Date
    Apr 2013
    Location
    Sydney
    Posts
    1,557

    Default

    After first coat? luck you.... try 2 weeks worth of 13coats, steel wool in between coats, perfect glass like finish then BAMMO!! warmish day, hundreds of unremovable blisters in the finish...... Odd as a smaller piece sitting right next to it, absolutely perfect...... go figure.

Similar Threads

  1. Replies: 3
    Last Post: 7th June 2015, 01:03 PM
  2. Two pot polyurethane varnish over urethane-alkyd varnish?
    By Theodor in forum BOAT BUILDING / REPAIRING
    Replies: 2
    Last Post: 4th October 2012, 10:07 PM
  3. last coat of varnish..........
    By Reiner in forum BOAT BUILDING / REPAIRING
    Replies: 16
    Last Post: 17th March 2010, 08:06 AM
  4. How to re-coat a floor with polyurethane
    By Extracare in forum FLOORING
    Replies: 11
    Last Post: 3rd April 2008, 09:45 AM
  5. Bubbles in new paintwork first coat
    By diymidget in forum PAINTING
    Replies: 1
    Last Post: 21st November 2007, 01:30 PM

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •