    I need some help please. I have Monocel timber varnish (gloss) and it just won't gloss, I went to the shop I bought it from and they said I need to stir it longer. I've tried a variety of different things such as mixing longer, applying with spray gun, brush, speedy pad, thinning it with turps and applying at different times of day in case temperature was a factor, but nothing works, I still get a matte appearance with 1 or 2 glossy spots. This is the first time I've used Monocel, my preferred varnish is no longer sold at my local paint store, I don't think the problem is timber related because I've had the same results on oak, mahogany, a real dark brown wood I think could be walnut and another unknown wood type (was trying to finish a few things at the same time).
    I've emailed the manufacturer to ask for advice and gave them the batch number in case the product is at fault, but I've had no reply.

    Please give me any advice/suggestions on how to stop getting a matte finish.

  2. # ADS
    Google Adsense Advertisement
    Join Date
    Always
    Location
    Advertising world
    Posts
    Many





     
  3. #2
    Join Date
    Feb 2009
    Location
    moonbi nsw Aus
    Age
    69
    Posts
    2,065

    Default

    You seem to have done all the right things.
    Usually there is 2 main reasons for lack of gloss and they are air temperature too low or damp air (high humidity/low temperature) causes "blushing".

    A matting paste is added to the mix to cut down on the level of gloss. It may be a miss labelled can? Only the manufacturer can help you there.

    Best of luck (very frustrating, I'll bet)
    Just do it!

    Kind regards Rod

  4. #3
    Join Date
    Jul 2013
    Location
    Hell
    Posts
    6

    Default

    Quote Originally Posted by chambezio View Post
    It may be a miss labelled can? Only the manufacturer can help you there.
    I've been wondering if the can may be mislabelled. I might just send the manufacturer another email.

    Quote Originally Posted by chambezio View Post
    (very frustrating, I'll bet)
    You have no idea.

    Thanks for your reply.

  5. #4
    Join Date
    Aug 2007
    Location
    Melbourne
    Posts
    2,178

    Default

    Hi DOgm4,

    How many coats are you applying? And to what grit did you sand the timber to before adding the Varnish?
    It's possible that you need to take the sanding up to 4-600 to get a good surface for this particular varnish. Also, you may find that sanding back between coats and reapplying several coats this way will bring up the gloss. Just a thought.

    Regards,

    Rob
    Last edited by LGS; 4th July 2013 at 02:42 PM. Reason: Typo

  6. #5
    Join Date
    Jul 2013
    Location
    Hell
    Posts
    6

    Default

    Quote Originally Posted by LGS View Post
    Hi DOgm4,

    How many coats are you applying? And to what grit did you sand the timber to before adding the Varnish?
    It's possible that you need to take the sanding up to 4-600 to get a good surface for this particular varnish. Also, you may find that sanding back between coats and reapplying several coats this way will bring up the gloss. Just a thought.

    Regards,

    Rob
    Hi Rob,

    Since I've been trying different solutions to get the gloss finish I'm up to 8 coats, after 24hr dry time I've sanded back each coat with 240. When the timber was bare I sanded it 180, 240, 320 and 400, then for first coat I added 25% turps as per manf. instructions. Normally I would only apply 3 coats.

    Thanks for your reply.

  7. #6
    Join Date
    May 1999
    Location
    Grovedale (Geelong) Victoria
    Age
    74
    Posts
    12,208

    Default

    Is there any cloudiness in the mix when it is stirred or is it dead clear?

    Full gloss should be clear where a mat or semi will have some cloudiness to it.

    Kinda sounds to me like you have a miss labelled tin.

    As a final thought... Not trying to be a smart, but are you sure you are adding mineral turpentine to the mix and not something else by mistake. This includes pure or gum turpentine which may not be suitable.

    Cheers - Neil

  8. #7
    Join Date
    Jul 2013
    Location
    Hell
    Posts
    6

    Default

    Quote Originally Posted by ubeaut View Post
    Is there any cloudiness in the mix when it is stirred or is it dead clear?

    Full gloss should be clear where a mat or semi will have some cloudiness to it.
    As a matter of fact, it does go cloudy when mixed. I didn't think anything of it, especially when the shop assistant said thorough mixing is required because all the "goodies" are at the bottom.

    Quote Originally Posted by ubeaut View Post
    Kinda sounds to me like you have a miss labelled tin.
    I'm convinced of this now. I emailed the manufacturer again yesterday but may have to use snail mail.

    Quote Originally Posted by ubeaut View Post
    As a final thought... Not trying to be a smart, but are you sure you are adding mineral turpentine to the mix and not something else by mistake. This includes pure or gum turpentine which may not be suitable.

    Cheers - Neil
    I use Diggers mineral turps. I didn't know there was a pure or gum turps so I've learned something new.

    Thanks for your reply.

  9. #8
    Join Date
    Jul 2013
    Location
    Hell
    Posts
    6

    Default

    I have a new question still related to this topic. Can I go out and buy a new can of gloss (different brand) and apply it directly over the Monocel varnish or would I need to sand right back to bare timber again? Can anyone recommend a good, inexpensive replacement brand? I used to use Wattyl Estapol but that's no longer stocked and I don't want to run the risk of getting another mislabelled/faulty product.

    Thanks.

  10. #9
    Join Date
    Dec 2010
    Location
    Melbourne
    Age
    79
    Posts
    601

    Default

    If you didn't use "pure turps" to thin (that will kill the gloss) the you have a faulty or mislabeled can take it back for an exchange.
    PS yes you can go over what you have ,just give it a light sand as normal
    Last edited by nrb; 6th July 2013 at 11:22 AM. Reason: more comment

  11. #10
    Join Date
    Jul 2013
    Location
    Hell
    Posts
    6

    Default

    Thanks for all your replies. Unfortunately I've misplaced my receipt and I can't pinpoint the exact day I bought the varnish, so the store doesn't want to go through an entire week's worth of eft-pos transactions looking for mine. I guess that's understandable.

    If I don't stir the varnish, will I be able to get a gloss finish that way?

Similar Threads

  1. Two pot polyurethane varnish over urethane-alkyd varnish?
    By Theodor in forum BOAT BUILDING / REPAIRING
    Replies: 2
    Last Post: 4th October 2012, 10:07 PM
  2. Replies: 2
    Last Post: 18th September 2011, 07:19 AM
  3. Matte Black pickguard material
    By Groundhangers in forum MUSICAL INSTRUMENTS
    Replies: 0
    Last Post: 25th August 2011, 11:48 PM
  4. How to apply gloss varnish properly?
    By wixy in forum FINISHING
    Replies: 7
    Last Post: 23rd August 2009, 09:36 PM
  5. Matte Gold BOWood
    By Penpal in forum WOODTURNING - PEN TURNING
    Replies: 5
    Last Post: 7th May 2008, 11:15 PM

Tags for this Thread

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •