I'm still struggling away with a project that has caused me to refettle my hand planes and learn to deal with difficult wood. The latest trial is I've had an edge joint on a panel break while cutting a housing joint with chisels. This happened on the first panel and I managed to reglue it thinking I just didn't put enough glue the first time. However, it has happened again on the second panel so I'm thinking something else might be going on and was after some help.
Some info:
It looks like the glue itself failed. I can't find any damage to the wood which is not what I believe I should expect for PVA (stronger than the wood?)
The glue I used is Parfix PVA from Bunnings that I've marked "Purchased 23/6/19". It's stored in a cupboard in the house but it may have been stored in a shed early on in its life.
I realised that my bench top was quite cupped which probably resulted in the board being flexed along the glue line each chisel strike. I've flattened that now
I thought I did a decent job of jointing the edges by hand but maybe not quite. I'm still not 100% confident in my abilities but had the joints not failed I thought I'd done an acceptable job. The earlier board would likely have had any gap in the middle. This second board on the ends and it started to fail there.
Some thoughts:
My glue could be old? It still looks like how PVA looks as far as I can tell so I'm not sure about this
My glue could just be not great and I should try a different brand. A forum search suggests some people dont rate parfix very highly at all.
The bench flatness issue likely exacerbated things. I haven't had any other failures so maybe I'm just stressing the joint more due to the bench.
My jointing and clamping might not have been perfect but surely I would've expected to see wood failure somewhere where there was no gap. There cant physically be a gap everywhere.
Some more questions:
Any other ideas?
If it's likely the glue, thoughts on Titebond (~18min drive away) or aquadhere (~8min drive)? Also the different types?
Any help would be appreciated
-
7th August 2023 04:09 PM # ADSGoogle Adsense Advertisement
- Join Date
- Always
- Location
- Advertising world
- Posts
- Many
-
7th August 2023, 08:13 PM #2
The other critical bit of info you haven’t mentioned is, what is the timber?
Cheers
DJ
ADMIN
-
7th August 2023, 09:32 PM #3GOLD MEMBER
- Join Date
- May 2011
- Location
- Albury
- Posts
- 3,052
Parfix PVA. Would not be surprised if there's a fair amount of extender (flour) in it. Unfortunately it's another case of you get what you pay for.
-
7th August 2023, 10:05 PM #4New Member
- Join Date
- Feb 2020
- Location
- Melbourne
- Posts
- 7
-
7th August 2023, 10:12 PM #5GOLD MEMBER
- Join Date
- May 2003
- Location
- Central Coast, NSW
- Posts
- 3,331
I have used Parfix PVA for years and have seen no indication that it is second rate.
I would not be using 4 year old glue - just in case.Apologies for unnoticed autocomplete errors.
-
10th August 2023, 08:32 AM #6New Member
- Join Date
- Feb 2020
- Location
- Melbourne
- Posts
- 7
I bought some aquadhere exterior. I'll see how I get along with it. I don't seem to be using enough that cost is a big issue tbh.
-
10th August 2023, 02:06 PM #7
Before I developed confidence in the tightness of my joints, I used slightly thickened epoxy as my go to glue. It's gap filling properties compensated for my deficiencies in craftsmanship.
PVA is not a gap filler so this might be an issue. The age of the glue could also be an issue. I have not had issues with gluing shining gum (aka nitens).
both Titebond and Aquadhere are good products - I don't know about Parfix. When you buy stuff from the super discounters, you will expect a high proportion to be crap, a small percentage are gems. One problem with Bunings is that they stock Good products and crap products side by side, and often their staff do not know the difference.
-
10th August 2023, 02:55 PM #8Senior Member
- Join Date
- Oct 2010
- Location
- Drouin Vic.
- Posts
- 166
One thing to keep in mind with all PVA emulsion based adhesives is they are made by polymerisation to produce polymer particles of various sizes suspended in a water base. With time gravity takes effect and the particles settle leaving a thin liquid layer on top which inside a glue bottle can be very hard to see and very difficult to re-disperse. This is especially the case with imported products such as my favorite Titebond which may well be 1 year old when sold at the retail level here in Australia.
Cheers,
Paintman
-
29th August 2023, 01:18 PM #9Senior Member
- Join Date
- Apr 2012
- Location
- Melbourne
- Posts
- 293
Aquadhere exterior should do the job.. bit messier to work with comparing to PVA.. but I never had any issues with it.. at one occasion I had 600 x 2000 x 45 board falling off the stand after being glued up.. timber cracked and split board in pretty much half length wise..but glue did not give up.. just applied glue to the crack line.. and clamped it again.. cant even see where the crack was..
-
29th August 2023, 02:23 PM #10
-
29th August 2023, 11:47 PM #11Senior Member
- Join Date
- Jun 2017
- Location
- Western Australia
- Posts
- 173
According to the Aquadhere website, Aquadhere Exterior is a PVA (it says it on the bottle).
-
30th August 2023, 01:39 AM #12SENIOR MEMBER
- Join Date
- Dec 2011
- Location
- SC, USA
- Posts
- 625
Please post some pics of the failed joints.
Ok, big misconception on glue... A properly prepped joint is typically stronger than the surrounding wood... BUT... The glue is not stronger by itself. All of us can attest to wide glue lines failing well before the wood.
Epoxy is one of the only glues that can tolerate some gap in the joint.
Typically "glue failures" are actually jointing failures.
A few things:
*Freshly prepped wood surfaces glue much better.
*Given equal jointing quality, planed joints are considerably stronger than sanded joints...
*But... A poorly prepped planed joint will be much worse than a well prepped sanded joint.
The #1 thing in studies tends to be the joint tightness prior to glue. Every 0.1mm of extra sliding clearance makes loose wobble which turns into a broken joint.
If you have a loose joint that you need to shore up, epoxy can be your friend. You need to use the good structural stuff used by sailboat guys, like West Systems. The wood still has to be carefully prepped immediately prior, and the epoxy prepared properly and applied to whet all the wood surfaces.
-
30th August 2023, 08:55 AM #13New Member
- Join Date
- Feb 2020
- Location
- Melbourne
- Posts
- 7
Unfortunately I didn't take any photos and have already reglued the joint.
I would have thought that I should have had good contact somewhere, it being an edge joint. However I don't recall finding any spot that looked like timber failure. Also, from some unrelated reading, I don't think any gap would have been bigger than what a spring joint would have. I could be wrong there though, both on memory of what I had and on how spring joints work.
I also can't recall if/how much I adjusted the fit when I was cleaning the dried glue off the edge of the boards
-
31st August 2023, 01:07 PM #14
Having contact somewhere is not enough. With most glues you must have contact virtually everywhere. The exceptions are the gap filling glues which essentially means epoxy.
A tiny bit of glue will fail before the timber; a moderate amount of glue will tear the timber out.
But if the glue itself is defective - long out of date or stored too hot - then it ain't glue anymore.
The questions that you are asking are all good; we have all been there ! The trick is to try not to repaet the same stuff ups too many times.
-
1st September 2023, 12:31 AM #15Member
- Join Date
- Feb 2023
- Location
- Finger Lakes Area, Central New York State, USA
- Age
- 69
- Posts
- 50
Re-gluing any joint is a risk. Glue works by bonding with the fiber of the wood. When a glue joint fails the original glue remains and adding new glue simply does not penetrate the wood blocked by the original glue. The joint will always be weak.
Without doubt this is a topic that could roll on forever but here are some Youtube links that might shed some light on the great end grain glue debate.
calabrese55
Glue Myths: 1. End grain https://www.youtube.com/watch?v=m7HxBa9WVis
End Grain Glue Myths | You May Have Misunderstood
End Grain Glue Myths | You May Have Misunderstood - YouTube
A misunderstanding of the end-grain glue "myth" video?
https://www.youtube.com/watch?v=dwLWmoGh59g
in general
https://www.youtube.com/results?sear...ng+glue+joints
Similar Threads
-
Planing For Edge Joint - How Best?
By abrogard in forum WOODWORK - GENERALReplies: 12Last Post: 14th February 2018, 09:43 AM -
Best glue for edge-to-edge kitchen worktop joint.
By Mike B in forum GLUEReplies: 8Last Post: 7th February 2015, 06:47 PM -
What preceded the edge-to-edge joint for creating large surfaces?
By Russell Cook in forum WOODWORK - GENERALReplies: 15Last Post: 25th November 2012, 04:22 AM -
How best to edge joint spooted gum slabs?
By Dengue in forum WOODWORK - GENERALReplies: 5Last Post: 15th September 2010, 08:33 AM -
Anyone Used a Glue Joint Bit for Table Top Glue-ups?
By TP1 in forum WOODWORK - GENERALReplies: 13Last Post: 25th March 2010, 11:28 PM